Steel Core Strength After Hardening & Tempering Temper. Temperature (N/mm2) Surface Hardness 90 Min 1076° F Melonite®
Name Steel Number 2 Hours 6 Hours HV 1 HV 10 HV 30
Ck15 1.1141 600 550 350 300 200
C45W3 1.1730 750 - 850 700 - 800 450 350 250
Ck60 1.1221 750 - 950 700 - 800  450  350  250 
20MnCr5 1.7147  800 - 950  800 - 900  600 450  400 
53MnV8 1.5141 850 - 950   800 - 900  450 400   350
90MnV8 1.2842 1000 - 1200   900 - 1100 550  450  400 
42CrMo4 1.7225 900 - 1200   900 - 1100 650   500 450 
X19NiCrMo4 1.2764  900 - 1100 900 - 1000  600  500  450 
55NiCrMov6 1.2713 1200 - 1400  1150 - 1300  650  550  500 
56NiCrMoV7 1.2714 1300 - 1500  1250 - 1400  650  550  500 
50NiCr13 1.2721 1200 - 1350  1100 - 1200  600  500  450 
X20Cr13 1.2082 1000 - 1200  1000 - 1200  > 900  600  450 
X35CrMo17 1.4122 1000 - 1200  1000 - 1200  > 900  700  550 
X210Cr12 1.2080 1500 - 1700  1400 - 1600  > 800  600  450 
X210CrW12 1.2436 1500 - 1800 1400 - 1650  > 800  600 500
X165CrMoV12 1.2601 1400 - 1900 1400 - 1700 > 800 650 500
45CrMoW58 1.2603 1500 - 1800 1400 - 1700 800 700 600
X32CrMoV33 1.2365 1700 - 1800 1600 - 1750 > 900 850 700
X38CrMoV51 1.2343 1700 - 1900 1500 - 1700 > 900 850 700
X37CrMoW51 1.2606 1700 - 1900 1600 - 1800 > 900 800 700
X30WCrV53 1.2567 1700 - 1900 1600 - 1800 > 900 850 750
X30WCrV93 1.2581 1500 - 1800 1500 - 1700 > 900 850 800